| NO. 序号 | Experiment Items 试验项目 | Experiment Method And Conditions 试验方法和条件 | Reference 参考文献 | 
| 1 | Solder Resistance Test 耐焊接热试验 | 265℃±5℃ for 10±2sec. Immerse body into solder 1/16''±1/32'' 将器件引线浸入熔融的260℃±5℃的焊料中10±2sec,浸至距离壳体1/16''±1/32'' 处 | JESD22-B106 JESD22-A111 | 
| 2 | Solderability Test 可焊性试验 | 245℃±5℃ for 5sec. 245℃±5℃,5秒 | J-STD-002 | 
| 3 | Salt Spray Test 盐雾试验 | 35±2℃,5% NaCl, 24H 试验温度:35±2℃,氯化钠盐水浓度:5%,24H | GB/T 2423.17-2008 | 
| 4 | ESD Test 抗静电试验 | 2KV (GPP/OJ/SKY>100V) 接触式,施加2KV,正负各10次 | IEC61000-4-2 | 
| 4KV (SKY=100V) 接触式,施加4KV,正负各10次 | 
| 8KV (SKY<100V) 接触式,施加8KV,正负各10次 | 
| 5 | High Temperature Reverse Bias Test 高温反偏试验 | Ta=100℃ for 1000hrs at VR=80%Rated VR (O/J) 在100℃情况下,施加80%的额定电压,1000小时(O/J/) | JESD22-A108 | 
| Ta=125℃ for 1000hrs at VR=80%Rated VR (DG) 在125℃情况下,施加80%的额定电压,1000小时(DG) | 
| Ta=150℃ for 1000hrs at VR=80%Rated VR (PG) 在150℃情况下,施加80%的额定电压,1000小时(PG) | 
| 6 | Forward Operation Life Test 正向工作寿命试验 | Ta=25℃ for 1000hrs at rated average rectified current 在25℃的情况下,通入额定电流,1000小时 | MIL-STD-750D METHOD-1027 | 
| 7 | Intermittent Operation Life Test 间歇工作寿命试验 | On state:5 min with rated IRMS power; Off state:5 min with cool forced air; On and Off for 1000 cycles 开态:额定功率5分钟; 关态:冷风吹5分钟; 共1000循环 | MIL-STD-750D METHOD-1036 | 
| 8 | Pressure Cooker Test 高压蒸煮试验 | 1.5 PSIG,Ta=121℃,96hrs 1.5 PSIG,Ta=121℃,96小时 | JESD22-A102 | 
| 9 | Temperature Cycling Test 温度循环试验 | -55℃/+150℃ 30 min for dwelled time 5 min for transfered time,total 500 cycles -55℃/+150℃,保持30分钟,转换时间5分钟,共500次循环 | JESD22-A104 | 
| 10 | Temperature Shock Test 冷热冲击试验 | -55℃ for 30min,150℃ for 30min,total 10 cycles -55℃保持30分钟,150℃保持30分钟,共10次循环 | MIL-STD-750D METHOD-1056 | 
| 11 | Forward Surge Test 正向浪涌试验 | 8.3ms single hale sine-wave one surge 8.3毫秒单向正弦半波 | MIL-STD-750 Method 4066 | 
| 12 | High-temperature High- humidity Reverse Bias 高温高湿反偏 | Ta=85℃,RH=85%,80%Rated VR for 1000hrs 85℃,85%相对湿度,1000小时 | JESD22-A101 | 
| 13 | High Temperature Storage Life Test 高温存储寿命试验 | 150℃ for 1000hrs 150℃,1000小时 | JESD22-A103 |